7696 Route 31, Lyons NY 14489 Tel: (315) 946-1213 Fax: (315) 946-4456
www.caswellplating.com sales@caswellplating.com
BLACK OXIDE KIT
NEW COLD SYSTEM
Professional Results In Minutes Simple Dip & Coat Method
The commercial gun blue manufacturers developed this new technique as a more environmentally friendly system
than the commonly used hot application. Parts requiring blackening are simply placed in the liquid at room
temperature. No electrical power is required.
Thoroughly clean the part to be blackened by sandblasting, wire brushing, wire wool abrasive cleaning, or by
scrubbing in VIM or COMET household abrasive cleaner. Make sure you have removed all rust, paint, oil and grease.
Thoroughly rinse prior to immersing into the concentrate.
Mix 1 Part Black Oxide Concentrate with 9 Parts Distilled Water in a plastic pail. Eg 1 Pint Black Oxide with 9 Pints
Distilled Water. Immerse the part in the mixed Black Oxide Solution and swirl around for between 30 seconds to 5
minutes maximum. Remove the part from the solution and rinse in fresh water. Smutting may occur when
immersed beyond 5 minutes.
Immediately brush on or dip the part into the Sealant and soak in the liquid for 1-2 minutes. Shake off any excess
and allow to dry thoroughly before handling. Note that the Penetrating Sealer leaves an oily finish and will not dry
completely.
Some hardened or specialized steels may not readily accept the blackening process. Activation can be done using
immersing in our Black Oxide Activator. Mix 1 Part Activator with 9 Parts Distilled Water. Immerse at room
temperature for 2 to 5 minutes, then thoroughly rinse before immersing into the black oxide. To enhance
blackening effect warm the part to approx. 120 degrees F, or warm the liquid to 120 degrees F before use.
Black Oxide Swab On Instructions
1. Degrease the area to be finished with a warm to hot soapy water. Do not use petroleum solvents as a
replacement.
2. Rinse with running water, a damp sponge or damp cloth. Apply the damp sponge or cloth for several
applications to thoroughly remove residual cleaning solution.
3. Remove any rust or welding scale with steel wool, abrasive paper or pad. Use a 10% sulfuric acid by
volume in water then rinse thoroughly.
4. CAUTION – Solution is Corrosive. Wearing gloves, apply the Black Oxide full strength generously with a
sponge, or cloth saturated with the solution and use a light rubbing action. Use care to insure a smooth
and even coverage. Allow the chemicals to react for 1 to 3 minutes. The depth of blackness is controlled
by the length of time the solution is left in contact with the steel surface. Repeated applications may be
required. The Black Oxide concentrated solution may be diluted with 2 to 4 parts distilled water to slow
down the blackening reaction when finishing large areas.
5. Rinse with running water, a damp cloth or damp sponge several times to remove residual blackening
solution. Adding a small amount of baking soda to the rinse water will help insure the complete removal of
the residual Black Oxide solution. If the residual solution is not completely removed, it may cause rusting
of the surface as it dries.
6. Wipe the area dry with a clean cloth and rub the area with soft cloths to remove any non-adherent layer of
spent chemicals.
7. Repeat steps 4, 5, and 6 if a darker finish is desired.
8. Apply Sealer.