Cerakote Instructions

Cerakote Instructions

                 TRAINING
                  MANUAL




      TRAINING VIDEOS AVAILABLE AT
    YOUTUBE.COM/NICTRAINING

WWW.CERAKOTEGUNCOATINGS.COM
             PLEASE READ
    Cerakote™ Firearm Coatings are designed for professionals
    and should be applied by NIC-trained applicators and coating
    professionals with proper training and equipment. This train-
    ing manual is intended to be used as a supplemental guide
    for certified and professional applicators ONLY. It is critical
    to follow all instructions in this manual. If for any reason you
    are not willing to, or cannot follow the steps in this manual,
    do not attempt to coat any product using Cerakote™, or any
    other NIC product. If you have any questions, please contact
    NIC Industries.

                              Thank you

                    Cerakote Firearm Coatings
                 A Division of NIC Industries, INC.
                           866-774-7628
                 www.CerakoteGunCoatings.com




1


               WWW.CERAKOTEGUNCOATINGS.COM
NOTES




                                  2


    WWW.CERAKOTEGUNCOATINGS.COM
     NOTES




3


    WWW.CERAKOTEGUNCOATINGS.COM
Phase 1: Disassemble
                         Disassemble:
               Completely disassemble the firearm.




       Detail strip your firearm. If you are unfamiliar with this
      level of disassembly have a certified gunsmith perform
                  the disassembly and reassembly.




     Take a photograph of all the parts received. Make note of
      the substrate type on each piece (i.e: Steel, Aluminum,
                 plastic, composite, polymer, etc.)                 4


         WWW.CERAKOTEGUNCOATINGS.COM
                         Phase 2: degrease


                                           Degrease:
    Soak each part for 10-15 minutes in a non-water based degreaser such as Brake-Kleen®
         (NIC Part # SE-174) or acetone. Spraying is not sufficient; soaking is required.
                              Allow parts to air dry after soaking.




         From this point on it is critical to avoid touching the parts with your bare hands.
                     Use powder-free latex style gloves to handle the parts.




5


                        WWW.CERAKOTEGUNCOATINGS.COM
Phase 3: surface-prep

                                      Surface Prep:
 Begin by plugging the bore at both the chamber and the muzzle end of the barrel prior
  to blasting. Grit blast the parts with #100 to #120 grit aluminum oxide or garnet sand
 at 80 to 100 psi. Strive for an even blast pattern over the surfaces of the parts. Lightly
            blast (30-40 psi) non-metal parts such as: wood, plastic or polymer.
                                                                          TIP:
                                                         • If the part’s surface is still shiny
                                                         after blasting, you haven’t blasted
                                                         enough.

                                                         • If you use too coarse of grit, the
                                                         microscopic valleys on the part’s
                                                         surface will be too deep for the 1.0
                                                         mil (.001”) coating to completely
                                                         fill while covering the correspond-
                                                         ing “peaks” sufficiently to assure a
                                                         satisfactory coating.

                                                         • Don’t use sand that has been
                                                         previously used to clean dirty,
                                                         greasy or oily parts. Doing so will
                                                         contaminate your parts.




                        CAUTION:
• If you use #120 grit, be sure the grit does not wear out
as you are using it. #120 is pretty fine at the start, and
will wear to an ineffective dust.

• Do not use glass beads. Glass beads dimple the sur-
face rather than etching it, and will not yield a sufficient
blast profile for optimum coating adhesion.                                                       6


                     WWW.CERAKOTEGUNCOATINGS.COM
                     Phase 4: racking/masking

                                        Racking:
    Hang or otherwise fixture your parts so that you can access all the surfaces of each
                                 part with your HVLP gun.
     *REMEMBER TO ALWAYS WEAR POWDER-FREE, LATEX-STYLE GLOVES.




                                  AR 15 Lower Receiver




                                    Correct Racking
                                      Techniques




    Remington 700 Receiver                                        Stripped Springfield 1911
                                                                           Frame




                                    Welding wire used to
                                      suspend parts
7


                     WWW.CERAKOTEGUNCOATINGS.COM
g   Phase 4: masking & racking supplies



               Recommended Masking & Racking Supplies:
      The following products can be purchased at www.CerakoteGunCoatings.com


           Cerakote Starter Racking,
            Masking and Camo Kit:
          Great starter kit with a starting
           quantity of racking, masking
              and camo products.
               NIC part # SE-175

                    Kit Includes
           -Various high temp plugs for
              nearly any caliber barrel
           -A variety of metal hooks for
              most racking situations
          -A small spool of racking wire
             -Three sizes of netting for
               overlay camo patterns
            -Various clamps for holding
                  netting in place




                                                     High Heat Tape:
                                              Used for masking areas where
                                               coating is not desired. Avail-
                                                  able in sizes 1/4” to 4”
                                                NIC part # SE-121 through
                                                          SE-127




                                                                                8


                       WWW.CERAKOTEGUNCOATINGS.COM
                      Phase 5: gas-out

                                       Gas-Out:
    After parts are racked, heat the parts in the oven at 250 degrees Fahrenheit (F) for
              30 minutes to drive off any remaining solvents or contaminants.




                                                       Remove the parts from the oven
                                                       and allow them to cool. If you see
                                                       any “wetness,” or other indica-
                                                       tion that oil was driven out of the
                                                       part, re-clean by soaking in the
                                                       degrease tank and reheat for an
                                                       additional thirty minutes. Any con-
                                                       tamination from this point onward
                                                       will result in a less than sastisfac-
                                                       tory finish. Be careful, and take
                                                       your time. If further degreasing is
                                                       required, repeat as necessary un-
                                                       til no wetness (oil) is visible.




9


                     WWW.CERAKOTEGUNCOATINGS.COM
Selecting the right series
for the application


              Selecting The Right Cerakote Series for the
                             Application.


                              Cerakote™ H-Series:
H-Series is the most durable of the standard Cerakote™ product and provides the best
performance in hardness, wear, scratch resistance, adhesion and rust resistance. It can
withstand temperatures up to 400 degrees F and comes in over 60 colors. H-Series is
a thermal cure finish and therefore should not be applied to optics and other items or
substrates which cannot be cured at the required temperatures. (See cure schedule
table, Page 16.)



                              Cerakote™ C-Series:
C-Series should ONLY be used for high-temp applications up to 1700 degrees F, such
as suppressors and machine gun barrels. C-Series is available in a wide range of colors
to match the overall finish requirement of the firearm or weapons system. C-Series is
used to coat scopes and other optics, as well as fiberglass, polymer and other substrates
which cannot be thermally cured.




                                                                                            10


                   WWW.CERAKOTEGUNCOATINGS.COM
                         Phase 6: coating prep

                                  Coating Preparation:
     Prepare the Cerakote for application. Begin by shaking the bottle until the coating is
     completely mixed, then shake some more for good measure. Determine how much Cera-
     kote you intend to use before mixing (see table 1 pg. 10) Pot life for mixed Cerakote is
     approximately two hours in an open container, and as much as four hours in a closed
     container. Consequently, mix only what you intend to use, to avoid wasted coating. (see
     usage chart pg. 10)




 1.) Pour the desired quantity      2.) Add hardener. Use table 1     3.) Mix thoroughly with a
of Cerakote into the graduated      pg. 10 to determine Cerakote               stir stick.
            cylinder.                 to hardener ratio for finish
                                                type.




                                                                       4.) Pour mixed coating
                                                                        through a disposable
                                                                     automotive type paint filter,
                                                                      or a reusable filter shown
                                                                         (NIC Part # SE-139)




11


                         WWW.CERAKOTEGUNCOATINGS.COM
Phase 6: coating prep

                      Coating Preparation Continued:
NOTE: If the proportions of Cerakote to Hardener are incorrect, or the combination of
Product and Hardener are not thoroughly mixed, the final product will be splotchy at best
because the coating mixture was uneven, and your work will be wasted.



                                       Table 1
                          Cerakote / Hardener Ratio

                           Matte Finish           24:1

                           Satin Finish           18:1

                           Semi Gloss             16:1




                              Table 2 (18:1 Ratio)
                    Cerakote / Hardener Ratio Usage Chart

         Firearm               Cerakote                       Hardener
                                mL/cc                          mL/cc
          Pistol                   36                              2
           Rifle                   72                              4

  **Read and follow the instructions that come with the color(s) you are using.
  Some Product to Hardener ratios are different depending on the color used.




                                                                                            12


                   WWW.CERAKOTEGUNCOATINGS.COM
                         Phase 7: Spraying

                                           Spraying

                                          CAUTION:
     Spray in a well-ventilated area, wear a respirator, protective gloves and safety glasses.
                Refer to the MSDS for additional safety and handling information



                           Final Checklist Before Spraying:
     • Plug or mask off all parts that are not to be coated. Remember Cerakote is applied
     at .001” which is very thin, most areas do not require masking, however, if you are
     unsure, contact NIC for assistance.

     • Ensure all parts to be coated are hung securely, ensuring parts do not touch
     anything during the application process

     • Do not coat springs as it is not recommended to heat springs during the curing
     process.

     • Plug the bore to prevent overspray inside the bore.




                                          PRACTICE:
            Practice spraying on a piece of metal before going on to your final project.
      A particularly good exercise is to spray and cure a few machine screws and matching
      nuts. You should be able to screw the nut onto the machine screw without difficulty. If
                           you can’t, you may be spraying too heavily.


13


                         WWW.CERAKOTEGUNCOATINGS.COM
Phase 7: mixing & Spraying supplies


                         Recommended Mixing
                          & Spraying Supplies
 NIC recommends the following products for the best results during the coating
                        prep and application process



                               Graduated Cylinder:
                               NIC Part # SE-147A (100 ml)
                               or NIC Part # SE-147B (50 ml)
                               Depending on coating volume.
                               NIC suggests using a 100M/L graduated cylinder for
                               accurate ratio measurements of Cerakote to hardener.




                                IWATA LPH-80:
                                NIC Part # SE-138
                                • Miniature, center post gravity feed spray gun is a full-
                                featured HVLP gun with spray characteristics similar to
                                Iwata’s popular RG-3 gun.

                                • Using only 1.8 cfm at 13 psi, this low-air-consumption gun
                                provides high atomization with precise control of the spray
                                pattern and a minimum of overspray.

                                • Features adjustable spray pattern from round to full-fan
                                shape.

                                • A stainless-steel nozzle, paint passage and heat-tempored
                                needle ensure long-lasting, peak-performance spraying.

                                • Uses the reliable and easy-to-service cartridge-style
                                “air-valve” set, which can be serviced outside the gun and
                                easily placed back into the gun body.

                                • Its 4 oz. (110 ml) stainless-steel gravity cup is center-
                                mounted and rotates, allowing for spraying horizontally,
                                vertically or underneath surfaces.

                                • Unlike siphon-feed guns, this gravity-feed cup will work
                                with small amounts of paint without spitting

                                • Spray pattern is from 1/8” to 6” (0.3 cm to 15.24 cm)       14


                WWW.CERAKOTEGUNCOATINGS.COM
                          Phase 7: spraying

                                   Spraying Continued:




                                                    Blow off parts with dry compressed air to
                                                  make sure there is no trapped media in holes
                                                   or pockets. Sand or other media left behind
                                                           will cause surface defects.




     Start spraying in the most difficult area of each
       part, then progress and finish to the easier
      areas. This should help avoid runs and thin
                          spots.




15


                         WWW.CERAKOTEGUNCOATINGS.COM
Phase 7: spraying

                             Spraying Continued:




 When spraying, strive for even coverage.
 You are seeking a 0.5 to 1.0 mil coating
 (0.0005” to 0.001”). Spray with sufficient
  volume that the Cerakote doesn’t “flash
    off” before the coating hits the part.
  When spraying, the part should appear
   wet but not so wet that it wants to run.




                                                             TIP:
                                              • Do not spray with a wide pattern.
                                              Doing so may cause dry spray or a
                                              rough finish.




   Example of “wetting out” the part                                                16


                 WWW.CERAKOTEGUNCOATINGS.COM
                         Phase 7: spraying

                                  Spraying Continued:




                                                     After each part is coated, set it aside
                                                    for about five to ten minutes. Cerakote
                                                      will still be wet to the touch until it is
                                                                     oven cured.
                                                     If you touch any coated parts before
                                                    curing, the coating will smudge and will
                                                              have to be refinished.




                                          “MISTAKES”
      If a mistake is made during spraying, e.g., a run, don’t attempt to wipe down the part
       and re-spray. Instead, rinse the part with cleaning solvent or acetone to completely
     remove the uncured coating. Re-blast the part, dry in the oven, blow off, and re-spray.




                                        Cleaning Up:
     Clean your tools with acetone. Contact NIC with questions regarding cleaning solvent
        compatibility. Discard any unused “mixed” Cerakote according to local and state
                 regulations. Do not return any unused “mix” to the bottle.



17


                        WWW.CERAKOTEGUNCOATINGS.COM
Phase 8: curing

                                    Oven Cure:
Carefully move each part into the oven and cure at 250 degrees (F) for two hours. If you
must hurry the process, curing for 45 minutes at 300 degrees (F) is an alternative cure
schedule. If the part(s) being coated are heat sensitive, 150 to 180 degrees (F) for two
hours will adequately cure plastic, polymer, wood and composite parts.

After curing is completed, remove the parts from the oven and allow the parts to cool.
Once parts are cool enough to handle, the firearm can be reassembled.

                                     **CAUTION**
If you are unsure as to the temperature stability of your parts, contact the manufacturer
prior to oven cure.




                           Cure Schedule Table
      Material            Temperature                          Time

        Metal
      (Standard)
                          250 Degrees F                       2 Hours

        Metal             300 Degrees F                     45 Minutes
     (Quick Cure)

        Metal
      (Flash, when        180 Degrees F                     15 Minutes
     using stencils)

        Wood,
        Plastic               150-180                         2 Hours
          or                 Degrees F
       Polymer



                                            TIP:
   • “Flashing” parts allows for partial curing at 180-200 degrees (F) for 15 minutes.
             This technique is used when applying and removing stencils.



                                                                                         18


                  WWW.CERAKOTEGUNCOATINGS.COM
                            training program

     Cerakote™ Firearm Coating Training Program
     NIC Industries offers the only one-on-one training program for Cerakote™ Firearm Coating. With indi-
     vidual training, our instructors speak with the customers prior to the training course to custom design
     each class to meet the specific needs of each customer. Customers can apply any of NIC’s industry
     leading firearm coatings on their own parts, or parts supplied by NIC. Courses are taught at NIC’s
     training facility in White City, Oregon, or onsite*. While every class is custom tailored to meet each
     customer’s needs, below are topics typically covered in most courses.

                                         Training Topics
      • Metal Prep                                       • Problem solving and troubleshooting defects

      • Out-gassing                                      • Proper equipment and operation

      • Racking Techniques                               • Re-works

      • Coating selection for various applica-           • Cost analysis
      tions
                                                         • Marketing
      • Basic to advanced ceramic application

      • Proper curing techniques and schedules

     *Contact NIC for further information about on-site training at 866-774-7628.




     Class Location

     NIC Industries, Inc. is located at 7050 Sixth Street, White City, OR, 97503. White City is located in
     Southern Oregon approximately 5 miles from Medford, Oregon, and approximately 280 miles from
     Portland, Oregon.

     Transportation

     Rogue Valley International Airport (MFR) is located 6 miles from NIC and provides daily flights from
     several major west coast airports. All major rental car companies are located at the Rogue Valley
     International Airport.

     Lodging

     NIC has negotiated discounted rates with several hotels in close proximity to our facility. Information
     can be found at http://www.cerakoteguncoatings.com/resource/downloads/




19


                           WWW.CERAKOTEGUNCOATINGS.COM
technical information

           H-Series CERAKOTE™ Firearm Coatings
The unique formulation used for Cerakote™ firearm coating enhances a number of physical perfor-
mance properties including: abrasion/wear resistance, corrosion resistance, chemical resistance,
impact strength, and hardness. Each of these properties is rigorously tested to guarantee that
Cerakote™ products remain at the forefront of the firearm coatings market. For this study, the
performance properties of Cerakote™ H-146 Graphite Black were compared to the products of two
firearm coatings competitors, denoted as C1 and C2. Each coating was evaluated on nine important
aspects including performance and cost. These results are summarized in table 1, shown below,
and a more extensive description is given in the following paragraphs.


      Table 1. Performance comparison of Cerakote™ H-146 to competitor firearm coatings, C1 and C2.
          Specification                    Cerakote™                  C1                        C2

      Taber Abrasion Testing          Wear cycles per mil:    Wear cycles per mil:   Wear cycles per mil:
         (ASTM D4060)                        6000                    597                    418


         Corrosion Testing            Corrorsion-free at:     Onset of Corrosion:     Onset of Corrosion:
          (ASTM B117)                    1000 hours              100 hours                45 hours

         Pencil Hardness
         (ASTM D3363)
                                              9h                      9h                       7h

       Adhesion Cross-Cut Tape
           (ASTM D3359)
                                              5b                      5b                       5b
            Mandrel Bend
            (ASTM D522)                      32%                    32%                        32%
              Impact
           (ASTM D2794)                 160 inch-lbs            160 inch-lbs           140 inch-lbs

       Chemical Resistance                Excellent               Excellent                    Good

       Theoretical Coverage
       (ft2/gal at 1 mil thickness)          478                    250*                       321
              Cost ($/ft )2
                                           $0.62/ft2              $0.65/ft2               $0.99/ft2
         VOC Compliance               VOC compliant in all     Non Compliant           Non Compliant
                                          50 states
      *Theoretical coverage if applied according to manufacturers specifications of 0.5 mil.


 See all the test results at http://www.cerakoteguncoatings.com/testing/




                                                                                                            20


                          WWW.CERAKOTEGUNCOATINGS.COM
     technical information




21


     WWW.CERAKOTEGUNCOATINGS.COM
technical information




                                    22


      WWW.CERAKOTEGUNCOATINGS.COM
     technical information




23

     WWW.CERAKOTEGUNCOATINGS.COM
technical information




                                    24


      WWW.CERAKOTEGUNCOATINGS.COM
            DIVISIONS OF NIC INDUSTRIES, INC.

     TURN UP THE HEAT WITH CERAKOTE HIGH TEMP.
                                                  TM




              TM


     CERAKOTE IS ALSO THE INDUSTRY LEADER IN EXHAUST COATINGS.
                      www.CerakoteHighTemp.com




     IF YOU CAN CERAKOTE, YOU CAN POWDER COAT.
                                TM




      PRISMATIC POWDERS OFFERS THE WORLDS LARGEST SELECTION
               OF CUSTOM COLORED POWDER COATINGS.
                       www.PrismaticPowders.com




        GET THE LATEST NEWS, UPDATES,
                             VIDEOS,
                             OFFERS,
                             & MORE

25


             WWW.CERAKOTEGUNCOATINGS.COM
contact information

                           Need Help?
At any point during the Cerakote application you have a question,
          please contact Cerakote Firearm Coatings at:
                           NIC Industries, Inc.
                            7050 Sixth Street
                           White City, OR 97503

                          Phone: 541-826-1922
                         Toll Free: 866-774-7628
                     Email: info@nicindustries.com
                   Web: www.CerakoteGunCoatings.com
                           Fax: 541-826-6372

                You can also view training videos online at:
                      www.YouTube.com/nictraining

                      Follow us on Facebook at:
                www.Facebook.com/CerakoteGunCoatings


    Subscibe to Cerakote’s Newsletter via www.CerakoteGunCoatings.com
             to receive Cerakote news, information, and events.




                                                                        26


               WWW.CERAKOTEGUNCOATINGS.COM
FINISH STRONG
                                        TM




      Cerakote Firearm Coatings
   A Division of NIC Industries, INC.
             866-774-7628
   www.CerakoteGunCoatings.com